A stainless steel chimney liner should be selected from the flue-gas chemistry, normal and upset temperatures, condensation risk, structural arrangement and required service life. 304L may suit mild dry duty, 316L or 316Ti can improve resistance in many industrial exhaust systems, and 904L, duplex or higher alloys may be needed as chloride and acid severity increases. Rainbow can coordinate alloy selection with liner supports, thermal expansion, insulation, fabrication and installation for a complete chimney system.
“Stainless steel” is not one material. Different grades respond differently to acidic condensate, chlorides, high temperature, cyclic operation and welding. Increasing thickness cannot always compensate for selecting the wrong grade. EPC teams should define the complete process envelope first and then compare the material, construction and lifecycle cost.
A stainless steel chimney flue liner is the gas-contacting metallic cylinder or surface that carries flue gas and protects the structural shell from heat, corrosion and condensate. It may be a separate flue inside a steel or concrete structure, a stainless layer bonded to structural steel, or the inner wall of a double-wall chimney.
The liner is different from the load-bearing shell. A carbon-steel outer shell can resist wind, seismic and dead loads while a thinner stainless layer handles the process environment. This separation often reduces the amount of expensive corrosion-resistant material and makes liner inspection or replacement easier.
Stainless steel does not remove the need for insulation, drainage or corrosion analysis. Wet deposits, low-pH condensate, chlorides, crevices and unsuitable weld details can still cause pitting, crevice corrosion, stress-corrosion cracking or attack near heat-affected zones.
| Construction type | Description | Typical advantage | Main design concern |
|---|---|---|---|
| Independent rigid liner | A separate cylindrical flue supported inside a shell, tower or windshield | Clear separation of structural and gas-contact functions | Buckling, supports, guides and thermal growth |
| Sectional liner | Individual liner sections supported at intermediate floors | Controls accumulated vertical load and simplifies replacement | Expansion joints, drainage and gas-tight connections |
| Top-hung liner | The liner is suspended from a high-level support | Allows downward thermal movement | Suspension reliability and access |
| Stainless-clad plate | A thin stainless layer is metallurgically bonded to structural steel | Combines corrosion resistance with structural thickness | Edge details, welding procedure and clad continuity |
| Welded sheet lining | Thin stainless or alloy sheet is attached to a backing shell | Reduces solid-alloy material quantity | Weld integrity, trapped moisture and substrate condition |
| Double-wall inner liner | Stainless inner wall, insulation or air gap, and separate outer wall | Factory fabrication and thermal control | Joint sealing, supports, pressure and condensate drainage |
EN 13084-6:2025 covers base-supported, sectional and top-hung steel liners located within a load-bearing structure. It also applies to the flue-gas-contact side of single-wall chimneys. Flexible residential relining products are a different product category and normally do not define large industrial stack design.

304 and low-carbon 304L are widely available and easy to fabricate. They may suit dry or mildly corrosive exhaust when chlorides and acidic condensation remain limited. They should not be selected only because the gas is described as “clean.” Startup, shutdown and cold weather can create condensate even when normal operation is dry.
316L contains molybdenum and normally offers better resistance to localized corrosion than 304L in many chloride-bearing environments. Its low carbon content helps control sensitization during welding. 316Ti is titanium-stabilized and may be specified where the project needs resistance to intergranular attack after elevated-temperature exposure.
Neither grade is universal. High chloride concentration, severe acid condensate, deposits and crevices can exceed their corrosion resistance. The uploaded keyword list contains both “316 flue liner” and “316Ti chimney liner,” but the grade must follow verified chemistry rather than keyword popularity.
904L has higher nickel and molybdenum content than common 300-series grades and is used where sulfuric acid or localized corrosion is more demanding. Superaustenitic grades with higher molybdenum and nitrogen extend resistance further in aggressive chloride service.
Higher alloy content increases material and fabrication cost. It can still be economical when it prevents frequent repairs, coating renewal or unplanned shutdowns. Welding consumables, forming limits and availability should be confirmed before the grade is fixed.
Duplex grades combine austenitic and ferritic structures. Duplex 2205 offers higher strength than common austenitic stainless steels and improved resistance to chloride stress-corrosion cracking in suitable environments. Super duplex grades provide greater localized corrosion resistance for more severe exposure.
Fabrication needs strict control of heat input, filler metal, interpass temperature and post-weld cleaning. Poor welding practice can disturb the phase balance and reduce toughness or corrosion resistance. A Duplex 2205 stainless steel inner liner was used with a Q355B outer shell and axial sliding connection in a 60 m hazardous-waste incineration chimney.
Heat-resistant stainless grades are considered where oxidation at elevated temperature is the main concern. High-temperature resistance does not automatically mean strong resistance to low-temperature acid condensate. The design must evaluate both hot operation and the wet conditions that can occur during startup, shutdown or low load.
Severe wet flue gas desulfurization service, very low pH, high chloride concentration or combined acids may require higher nickel alloys, titanium, FRP or another lining system. The Nickel Institute describes a progression from 316L for mild conditions through higher-alloy stainless and duplex materials to nickel alloys for the most severe FGD environments.
| Grade family | Potential application range | Main strength | Main limitation |
|---|---|---|---|
| 304/304L | Mild, mainly dry exhaust | Availability and fabrication economy | Limited resistance to aggressive chlorides and acid condensate |
| 316L/316Ti | Boilers and industrial exhaust with moderate corrosion risk | Improved localized corrosion resistance over 304 | Can pit or crack in severe chloride and low-pH service |
| 904L/superaustenitic | More aggressive acid or chloride environments | Higher molybdenum and nickel content | Higher cost and specialist fabrication |
| Duplex 2205 | Corrosive service requiring strength and chloride SCC resistance | High strength and useful corrosion resistance | Welding and phase-balance control |
| Super duplex | Severe localized-corrosion environments | Greater pitting and crevice-corrosion resistance | Cost, availability and strict fabrication control |
| 309/310S | High-temperature oxidation service | Elevated-temperature performance | Not automatically suitable for acid condensation |
This table is a screening aid, not a material specification. Final selection should use measured or conservatively defined condensate chemistry, temperature profiles, deposits, cleaning media and comparable service references. The corrosion behavior of stainless steel is affected by chloride concentration, temperature, surface condition, oxygen, pH and crevice geometry.

Stainless liners are used where boiler or generator exhaust can condense or where carbon steel would need frequent coating maintenance. The design should coordinate fuel, sulfur level, exhaust temperature, operating cycle, silencer and duct loads, insulation, backpressure and drain locations.
Waste combustion can produce chlorides, sulfur compounds, moisture and variable temperatures. Material selection should use the treated gas composition at the chimney inlet, not only the furnace fuel list. Incineration projects may use 316L, duplex or higher alloys depending on the actual process and air-pollution-control system.
Wet scrubbers lower flue-gas temperature and can create saturated, acidic and chloride-bearing conditions. Stainless, duplex, superaustenitic and nickel alloys may be considered by severity. Drainage, deposit control and avoidance of crevices are as important as the nominal alloy grade.
These facilities may combine acids, alkalis, chlorides, dust, washing cycles and process upsets. The supplier needs gas and condensate analysis from the specific process. A generic statement such as “chemical exhaust” is not enough to select an alloy.
A stainless inner flue can be installed inside a carbon-steel shell, steel tower or concrete windshield. The broader industrial steel chimney system must coordinate liner reactions, guides, platforms, duct interfaces, vibration control and future removal routes.
Record minimum, normal, maximum and excursion temperatures, including excursion duration. Add flow, pressure, moisture, oxygen, sulfur oxides, chlorides, fluorides, particulate, acid dew point and condensate pH. Include startup, shutdown, low load, scrubber trip, washing and bypass operation.
Calculate or assess the liner wall-temperature profile instead of relying only on bulk gas temperature. Cold bridges, expansion joints, the stack top, access doors and the lower inlet region can create local condensation. Deposits can concentrate chlorides or acids beyond the bulk gas analysis.
Determine whether the controlling risk is uniform acid attack, pitting, crevice corrosion, stress-corrosion cracking, intergranular attack, erosion-corrosion or high-temperature oxidation. Select candidate grades using qualified corrosion data and comparable references, then test where the chemistry is unusual.
Solid stainless construction is straightforward but uses more alloy. Clad plate combines a structural backing with a corrosion-resistant surface. Welded sheet lining reduces alloy volume but creates many attachment and seal welds. Compare total installed cost, inspection access and repairability—not plate price alone.
Stainless liners and carbon-steel shells expand differently. Base supports, sectional floors, guides, sliding connections and expansion joints must follow one movement model. Over-restraint can buckle the liner or overload supports; insufficient guidance can permit vibration and contact with the shell.
The welding procedure should match the grade and service. Control filler metal, heat input, interpass temperature, distortion, purge where required, weld profile and inspection. Remove contamination and damaging heat tint as specified. Rough welds, crevices and embedded carbon steel can become local corrosion sites.
An insulated stainless steel chimney liner can reduce heat loss and condensation during selected operating cases, but insulation cannot eliminate wet-service risk in every condition. Provide drains, wash-down access, inspection doors and platforms where condensate or deposits are expected.
Include engineering, alloy quantity, fabrication, welding, inspection, transport, erection, planned outage, cleaning, repair and replacement. A higher alloy may be justified in a critical wet zone while a lower grade remains suitable elsewhere. Zoning materials can reduce cost if every transition is properly detailed.

ASME STS-1:2026 is the current ASME steel-stack edition shown by the standards body. Its scope covers steel stacks with lined or unlined, single- or multiple-wall construction, along with material selection, linings, coatings, structural design, inspection and maintenance.
EN 13084-6:2025 addresses steel lining systems for free-standing chimneys. European projects may also need related Eurocodes, execution standards, material standards, national annexes and product conformity requirements.
The contract must state the governing standard, edition and component boundaries. Do not combine partial factors, load combinations or acceptance criteria from different systems without an approved design basis.
Writing only “stainless steel”: state the exact grade, product form, thickness and applicable material standard.
Selecting from temperature alone: chloride and acid condensation often govern corrosion.
Assuming thicker 304 equals a higher alloy: extra thickness does not provide the same resistance to localized corrosion.
Ignoring upset conditions: bypass temperature or scrubber failure may govern the design.
Using bulk chemistry only: deposits, crevices and evaporation can create more severe local conditions.
Leaving weld quality undefined: filler, heat input, cleaning and inspection affect corrosion performance.
Forgetting external liner surfaces: water in the annular space can corrode the liner from outside.
Using insulation as the only corrosion measure: shutdown and low-load operation can still create condensate.
A technical RFQ should include:
Chimney height, liner diameter, number of flues and support arrangement
Gas flow, pressure and allowable backpressure
Normal, minimum, maximum and excursion temperatures
Gas composition, moisture, particulate and condensate analysis
Acid dew point and expected wet or dry operation
Required stainless grade, thickness or performance criteria
Structural loads, expansion range, supports and guides
Insulation, drainage, access and cleaning method
Welding procedures, surface treatment, NDT and leak testing
Governing standards, editions, inspection plan and documentation
Material choice should also be checked against actual fabrication and installation capability. The corrosion-resistant design of industrial steel chimneys must connect alloy selection with coatings, insulation, drainage and maintenance access rather than treating the liner as an isolated purchase.
No. 316L generally offers improved localized corrosion resistance because it contains molybdenum, but the correct grade depends on chemistry, temperature and cost. Mild dry service may not need 316L, while severe wet chloride service may exceed its capability.
316L uses low carbon content to reduce sensitization risk during welding. 316Ti is stabilized with titanium for resistance to intergranular corrosion after certain elevated-temperature exposures. The choice should follow the applicable material standard, fabrication process and expected temperature cycle.
Duplex 2205 may be considered when a liner needs higher strength and improved resistance to chloride stress-corrosion cracking and localized corrosion. It still needs chemistry verification and tightly controlled welding because unsuitable heat input can damage phase balance and performance.
Yes. Stainless steel can suffer pitting, crevice corrosion, stress-corrosion cracking, intergranular attack and weld-area corrosion. Risk increases with chlorides, low pH, high temperature, deposits, evaporation, crevices and unsuitable fabrication or cleaning practices.
Often, but not automatically. Insulation can control heat loss, shell temperature and condensation during defined operating cases. It may also hide external corrosion if water enters the annular space. Thermal analysis, drainage and inspection access should be designed together.
Yes. Material zoning can place a higher alloy in wet or chemically severe areas and a lower grade in milder zones. Every transition needs compatible welding, galvanic review, thermal-movement detailing and clear inspection access, so zoning is an engineered solution rather than a purchasing substitution.
Inspection may include visual testing, liquid penetrant testing, radiographic or ultrasonic testing where applicable, dimensional checks and leak testing. The inspection plan should match the weld category, liner pressure, grade, thickness, governing code and consequence of leakage.
Provide gas and condensate chemistry, moisture, dust, pressure, normal and upset temperatures, acid dew point, operating cycles, washing chemicals, required life and expected inspection intervals. Without these inputs, a grade recommendation is preliminary and should not be treated as final.